Posted: Tue Oct 03, 2006 7:49 am Post subject: Alodine spar |
|
|
I am looking at corrosion resistance on My new spars. I have some alodine
from the local auto parts store. Clearly the instructions assume I will
simply slosh some of this back and forth inside the tube. Other instructions
I have read about alodine seem to want some fairly aggressive scrubbing
first. How have you done it? Thanks.
| - The Matronics Kitfox-List Email Forum - | | Use the List Feature Navigator to browse the many List utilities available such as the Email Subscriptions page, Archive Search & Download, 7-Day Browse, Chat, FAQ, Photoshare, and much more:
http://www.matronics.com/Navigator?Kitfox-List |
|
|
|
Back to top |
|
 |
Guy Buchanan

Joined: 16 Jul 2006 Posts: 1204 Location: Ramona, CA
|
Posted: Tue Oct 03, 2006 1:56 pm Post subject: Alodine spar |
|
|
At 08:49 AM 10/3/2006, you wrote:
Quote: | Clearly the instructions assume I will
simply slosh some of this back and forth inside the tube. Other instructions
I have read about alodine seem to want some fairly aggressive scrubbing
first. How have you done it?
|
I always use Metl-Prep before Alodine. It's available at ACS and it
chemically etches the aluminum.
Guy Buchanan
K-IV 1200 / 582-C / Warp / 100% done, thanks mostly to Bob Ducar.
| - The Matronics Kitfox-List Email Forum - | | Use the List Feature Navigator to browse the many List utilities available such as the Email Subscriptions page, Archive Search & Download, 7-Day Browse, Chat, FAQ, Photoshare, and much more:
http://www.matronics.com/Navigator?Kitfox-List |
|
_________________ Guy Buchanan
Deceased K-IV 1200
A glider pilot too. |
|
Back to top |
|
 |
janderson412(at)hotmail.c Guest
|
Posted: Tue Oct 03, 2006 2:20 pm Post subject: Alodine spar |
|
|
You need to slightly scuff the surface first. I used a wod of scotch bright
and dragged it back and forth with a light rope, then plug one end and slosh
out with the alodine.
From: "Dave G." <occom(at)ns.sympatico.ca>
Reply-To: kitfox-list(at)matronics.com
To: <kitfox-list(at)matronics.com>
Subject: Alodine spar
Date: Tue, 3 Oct 2006 12:49:10 -0300
I am looking at corrosion resistance on My new spars. I have some alodine
from the local auto parts store. Clearly the instructions assume I will
simply slosh some of this back and forth inside the tube. Other instructions
I have read about alodine seem to want some fairly aggressive scrubbing
first. How have you done it? Thanks.
_________________________________________________________________
Discover fun and games at (at) http://xtramsn.co.nz/kids
| - The Matronics Kitfox-List Email Forum - | | Use the List Feature Navigator to browse the many List utilities available such as the Email Subscriptions page, Archive Search & Download, 7-Day Browse, Chat, FAQ, Photoshare, and much more:
http://www.matronics.com/Navigator?Kitfox-List |
|
|
|
Back to top |
|
 |
shilocom(at)mcmsys.com Guest
|
Posted: Wed Oct 04, 2006 3:24 am Post subject: Alodine spar |
|
|
Alodine is a Chemical etch and only requires contact and time to get the job
done. That being said, I know others believe it is a "corrosion inhibitor",
I believe that is wishful thinking. None of the tech sheets make any such
claims that I've seen. It is simply an etch for improved paint adhesion and
not much more if anything. Dupont recommends the acid wash first then the
alodine. Alodine has been on there long enough and your acid prep was good
enough when it turns the metal a dark yellow. Self etching epoxy primers
do the same thing in one step. That's what I use now. Bob U.
---
| - The Matronics Kitfox-List Email Forum - | | Use the List Feature Navigator to browse the many List utilities available such as the Email Subscriptions page, Archive Search & Download, 7-Day Browse, Chat, FAQ, Photoshare, and much more:
http://www.matronics.com/Navigator?Kitfox-List |
|
|
|
Back to top |
|
 |
Float Flyr

Joined: 19 Jul 2006 Posts: 2704 Location: Campbellton, Newfoundland
|
Posted: Wed Oct 04, 2006 5:57 am Post subject: Alodine spar |
|
|
Scrub and Alumiprep first until water will sheet off the part. (water brake
test) rinse and immediately alodine. In a nutshell that's how I did it.
Noel
[quote] --
| - The Matronics Kitfox-List Email Forum - | | Use the List Feature Navigator to browse the many List utilities available such as the Email Subscriptions page, Archive Search & Download, 7-Day Browse, Chat, FAQ, Photoshare, and much more:
http://www.matronics.com/Navigator?Kitfox-List |
|
_________________ Noel Loveys
Kitfox III-A
Aerocet 1100 Floats |
|
Back to top |
|
 |
occom
Joined: 26 Aug 2006 Posts: 404
|
Posted: Wed Oct 04, 2006 8:02 am Post subject: Alodine spar |
|
|
---
| - The Matronics Kitfox-List Email Forum - | | Use the List Feature Navigator to browse the many List utilities available such as the Email Subscriptions page, Archive Search & Download, 7-Day Browse, Chat, FAQ, Photoshare, and much more:
http://www.matronics.com/Navigator?Kitfox-List |
|
|
|
Back to top |
|
 |
janderson412(at)hotmail.c Guest
|
Posted: Wed Oct 04, 2006 2:17 pm Post subject: Alodine spar |
|
|
I am told by one of our aviation technical staff that in laymen’s terms it's
a neutralizing coating, sort of satisfies the surface neutrons desire to
look for another (oxidizing) brother neutron. "Corrosion inhibitor", well
it’s debatable, again he said if undisturbed, yes. Look at the many alloy
alodined components that are stored for years before use with no corrosion
showing, but one small scratch and it will corrode . The paint over top of
raw aluminum alloy is not a corrosion inhibitor, it’s just a coating, (some
etch coatings may be) but by alodining the combination will offer more
pertinent protection.
From: "Bob Unternaehrer" <shilocom(at)mcmsys.com>
Reply-To: kitfox-list(at)matronics.com
To: <kitfox-list(at)matronics.com>
Subject: Re: Alodine spar
Date: Wed, 4 Oct 2006 06:33:37 -0500
Alodine is a Chemical etch and only requires contact and time to get the job
done. That being said, I know others believe it is a "corrosion inhibitor",
I believe that is wishful thinking. None of the tech sheets make any such
claims that I've seen. It is simply an etch for improved paint adhesion and
not much more if anything. Dupont recommends the acid wash first then the
alodine. Alodine has been on there long enough and your acid prep was good
enough when it turns the metal a dark yellow. Self etching epoxy primers
do the same thing in one step. That's what I use now. Bob U.
---
| - The Matronics Kitfox-List Email Forum - | | Use the List Feature Navigator to browse the many List utilities available such as the Email Subscriptions page, Archive Search & Download, 7-Day Browse, Chat, FAQ, Photoshare, and much more:
http://www.matronics.com/Navigator?Kitfox-List |
|
|
|
Back to top |
|
 |
janderson412(at)hotmail.c Guest
|
Posted: Wed Oct 04, 2006 2:35 pm Post subject: Alodine spar |
|
|
Sorry, I meant permanent protection....
I am told by one of our aviation technical staff that in laymen’s terms it's
a neutralizing coating, sort of satisfies the surface neutrons desire to
look for another (oxidizing) brother neutron. "Corrosion inhibitor", well
it’s debatable, again he said if undisturbed, yes. Look at the many alloy
alodined components that are stored for years before use with no corrosion
showing, but one small scratch and it will corrode . The paint over top of
raw aluminum alloy is not a corrosion inhibitor, it’s just a coating, (some
etch coatings may be) but by alodining the combination will offer more
permanent protection.
From: "Bob Unternaehrer" <shilocom(at)mcmsys.com>
Reply-To: kitfox-list(at)matronics.com
To: <kitfox-list(at)matronics.com>
Subject: Re: Alodine spar
Date: Wed, 4 Oct 2006 06:33:37 -0500
Alodine is a Chemical etch and only requires contact and time to get the job
done. That being said, I know others believe it is a "corrosion inhibitor",
I believe that is wishful thinking. None of the tech sheets make any such
claims that I've seen. It is simply an etch for improved paint adhesion and
not much more if anything. Dupont recommends the acid wash first then the
alodine. Alodine has been on there long enough and your acid prep was good
enough when it turns the metal a dark yellow. Self etching epoxy primers
do the same thing in one step. That's what I use now. Bob U.
---
| - The Matronics Kitfox-List Email Forum - | | Use the List Feature Navigator to browse the many List utilities available such as the Email Subscriptions page, Archive Search & Download, 7-Day Browse, Chat, FAQ, Photoshare, and much more:
http://www.matronics.com/Navigator?Kitfox-List |
|
|
|
Back to top |
|
 |
occom
Joined: 26 Aug 2006 Posts: 404
|
Posted: Sat Oct 07, 2006 9:50 am Post subject: Alodine spar |
|
|
Quote: | >
> <shilocom(at)mcmsys.com>
>
> Alodine is a Chemical etch and only requires contact and time to get the
> job
> done. That being said, I know others believe it is a "corrosion
> inhibitor",
> I believe that is wishful thinking. None of the tech sheets make any
> such
> claims that I've seen. It is simply an etch for improved paint adhesion
> and
|
Hi Bob and list. I picked up the product I bought and while I had asked for
Alodine by name the product I received is Dupont 225S metal prep and Dupont
226S Conversion Coating which does contain chromic acid and is advised to
give a high degree of corrosion resistance on aircraft etc. Says it
stabilizes aluminum and give corrosion resistance and paint adhesion. It may
be the same as Alodine as it says it imparts a "golden" colour. We'll see. I
may ultimately wash the inside if the spars with zinc chromate or epoxy
chromate but the original spars lived in our Maritime climate for 15 years
and there is no sign of any corrosion on the pile of cut up spar.
| - The Matronics Kitfox-List Email Forum - | | Use the List Feature Navigator to browse the many List utilities available such as the Email Subscriptions page, Archive Search & Download, 7-Day Browse, Chat, FAQ, Photoshare, and much more:
http://www.matronics.com/Navigator?Kitfox-List |
|
|
|
Back to top |
|
 |
janderson412(at)hotmail.c Guest
|
Posted: Sat Oct 07, 2006 12:30 pm Post subject: Alodine spar |
|
|
Sounds the same as Alodine if it contains chromic acid, and offers corrosion
resistance but to just the surface layer. Do not scratch or scuff after
treatment, just degrease.
From: "Dave G." <occom(at)ns.sympatico.ca>
Reply-To: kitfox-list(at)matronics.com
To: <kitfox-list(at)matronics.com>
Subject: Re: Alodine spar
Date: Sat, 7 Oct 2006 14:49:26 -0300
Quote: | >
><shilocom(at)mcmsys.com>
>
>Alodine is a Chemical etch and only requires contact and time to get the
>job
>done. That being said, I know others believe it is a "corrosion
>inhibitor",
>I believe that is wishful thinking. None of the tech sheets make any such
>claims that I've seen. It is simply an etch for improved paint adhesion
>and
|
Hi Bob and list. I picked up the product I bought and while I had asked for
Alodine by name the product I received is Dupont 225S metal prep and Dupont
226S Conversion Coating which does contain chromic acid and is advised to
give a high degree of corrosion resistance on aircraft etc. Says it
stabilizes aluminum and give corrosion resistance and paint adhesion. It may
be the same as Alodine as it says it imparts a "golden" colour. We'll see. I
may ultimately wash the inside if the spars with zinc chromate or epoxy
chromate but the original spars lived in our Maritime climate for 15 years
and there is no sign of any corrosion on the pile of cut up spar.
_________________________________________________________________
Discover fun and games at (at) http://xtramsn.co.nz/kids
| - The Matronics Kitfox-List Email Forum - | | Use the List Feature Navigator to browse the many List utilities available such as the Email Subscriptions page, Archive Search & Download, 7-Day Browse, Chat, FAQ, Photoshare, and much more:
http://www.matronics.com/Navigator?Kitfox-List |
|
|
|
Back to top |
|
 |
Fox5flyer Guest
|
Posted: Sun Oct 08, 2006 3:41 am Post subject: Alodine spar |
|
|
I used Alodine on some aluminum parts, but wasn't impressed. After a
year or so the paint began to peel off in places. I cleaned and
scotch brighted according to directions. I've had much better luck
with the old tried and tested zinc chromate, and better luck with
epoxy chromate. A good cleaning and scotch brighting is necessary
prior to application. I try to get it covered within 4 hours of
cleaning because aluminum oxidizes very quickly.
Deke
--
| - The Matronics Kitfox-List Email Forum - | | Use the List Feature Navigator to browse the many List utilities available such as the Email Subscriptions page, Archive Search & Download, 7-Day Browse, Chat, FAQ, Photoshare, and much more:
http://www.matronics.com/Navigator?Kitfox-List |
|
|
|
Back to top |
|
 |
|
|
You cannot post new topics in this forum You cannot reply to topics in this forum You cannot edit your posts in this forum You cannot delete your posts in this forum You cannot vote in polls in this forum You cannot attach files in this forum You can download files in this forum
|
Powered by phpBB © 2001, 2005 phpBB Group
|